PROPERTIES |
TEST METHOD |
UNITS |
STANDARD |
MEASURE |
| DENSITY | ASTM D792 |
gr/cm³ |
1.32 |
|
| HARDNESS | ASTM D 2240 |
SHORE A |
93 |
|
| TENSILE STG. | ASTM D 638 |
n/mm² |
15.0 |
20 |
| ELONGATION | ASTM D 638 |
%þ |
150.00 |
280 |
| THERMAL STAB. | 200°C |
minutes |
240` |
400 |
| FLAME RETARDANT | UL 94 |
V1 |
PROPERTIES |
TEST METHOD |
UNITS |
STANDARD |
MEASURE |
| TENSILE STG.min. |
ASTM D638 |
N/mm² |
15 |
18 |
| Variation max. |
%þ |
+/- 25 % |
-10 |
|
| ELONGATION min. |
ASTM D638 |
%þ |
þ þ150 |
250 |
| Variation max. |
%þ |
+/- 25 % |
-12 |
|
| LOSS of MASS | BS 6469 |
|||
| Variation max. |
115C/336H |
mg/cm² |
-1.5 |
-1.2 |
| THERMAL STAB. | minutes |
120 |
175 |
PROPERTIES |
TEST METHOD |
UNITS |
STANDARD |
RESULT |
| SPECIFIC RESISTANCE | OHM*CM |
20°C |
7.5* 1013 |
|
| SPECIFIC RESISTANCE | OHM*CM |
60°C |
1.4* 1012 |
|
| SPECIFIC RESISTANCE | OHM*CM |
90°C |
1.4* 1011 |
|
| DIELECTRIC STRENGTH | KV/mm |
27.8 |
||
| DIELECTRIC FACTOR | 1000Hz |
0.0638 |
||
| DIELECTRIC CONSTANT | 1000Hz |
4.9 |